Bearing SelectorPick the right bearing, step by stepVerify a BearingLife, safety factor and fitsLoad CalculatorLoads from your machineWorked templatesFan, gear and shaft load templatesCross-ReferenceNewSame size from other makers. Free, no sign-upBearing AutopsyNewUpload a photo, get the likely causesFailure AnalysisRead damage, find the causeCondition MonitoringVibration, envelope, oil clues, RCMLubricationGreases, oils, cleanliness, oil lifePM criticalityScore assets, set the PM orderEquipment AnatomyMotors, pumps, fans, gearboxesFAQ and quick checksSearch the basics in plain languageFind a DistributorSuppliers by brand and city

Learn

Free calculatorsLife, grease, oil, loads and moreFind a bearingSize, rating and equivalents by designationFailure modesDamage types, causes and fixesBearing materialsSteels, heat treatment, ceramicsCondition monitoringVibration, envelope, oil clues, RCMKnowledge libraryLubrication and reliability articlesBearings by machineMotors, pumps, mills, kilns and moreHow-to guidesBearing life, grease, failures, numbersShaft alignmentSoft foot, procedure, tolerances, heatField casesFailure investigations and monitoring cases (licence)Lubrication guidesGreases, oil systems, oil life and costPM criticality matrixRank assets by what a failure costsQuick answersPlain-language answers to common questions

Play

PlaygroundLearn engineering by playing with it

More

PricingPartnershipsExpertsContact
Materials

Bearing materials: steels, heat treatment and ceramics compared

Quick answer

For most duties the standard 100Cr6 steel is right. Change the material only when a specific problem calls for it: heat, dirty lubricant, shock, sliding, corrosion, dry running or electric current. The tables below show what each option is good at, compared with the standard steel.

By Tanmay Sharma, founder of Rotec AI. Qualitative guide for choosing and checking bearing materials; confirm any critical selection with your bearing supplier.

How the materials compare

Each row is scored against the standard bearing steel, 100Cr6 martensitic (the reference). A plus is better, an equals sign is the same, and a minus is worse. Scores are qualitative and the price column is only a guide, because real prices depend on the product and the quantity.

Standard solutions

Material and heat treatmentFatigueThermal influencesSliding (slippage) loadMechanical shockParticle overrollingCorrosionPrice
100Cr6, martensitic, class SN (reference 1)=−====Reference
100Cr6, martensitic, class S0 (reference 2)======Reference
100Cr6, martensitic, class S1=++−−−−Same
100Cr6, bainitic, class S1+++++−Same
St4 low-carbon steel, case hardened−−====Same
100CrMnSi6-4, modified martensitic+===+=Slightly higher
100CrMnSi6-4, carbonitrided++−+=++−Slightly higher
Case-hardening steel, case hardened+=++++−Slightly higher
Case-hardening steel, carbonitrided++=++++−Slightly higher
Nitrogen-alloyed corrosion-resistant steel (X30CrMoN15-1)+++= to ++++=++++Higher
Corrosion-resistant case-hardened nitrogen steel+=+==++Slightly higher

Special solutions

Material and heat treatmentFatigueThermal influencesSliding (slippage) loadMechanical shockParticle overrollingCorrosionPrice
100Cr6, martensitic, class SN (reference 1)=−====Reference
100Cr6, martensitic, class S0 (reference 2)======Reference
M50 tool steel, martensitic=++==−−Higher
M50NiL, case hardened+++++++++−Higher
Austenitic stainless, carburised−+==−+Higher
M50NiL, duplex hardened++++++++++−Much higher
32CrMoV13, nitrided+++++++++=Slightly higher
Powder-metallurgy high-speed steel+++++++++++++=Higher
Hard metal (cemented carbide, metallic binder)++++++++=++++++Much higher
Silicon nitride Si3N4 (rolling elements)++++++==++Much higher
Zirconium oxide ZrO2 (rolling elements)−+++=−−+++Higher
SymbolCompared with the reference
+++Excellent
++Significantly better
+Better
=Identical to the reference
−Worse
−−Significantly worse

Through-hardened and standard steels

The everyday rolling bearing steels. 100Cr6 is hardened right through and tempered; the tempering temperature sets the stabilisation class (SN, S0, S1), which is how far above normal the ring keeps its size when hot. Bainitic hardening and low-carbon formed-part steel complete the family.

MaterialHardness and temperatureStrengthsLimitsTypical uses
100Cr6 martensitic, class SNHardness up to 64 HRC; to about +120 °CVersatile, very hard, wear resistant, resists overrolling; best price and performance; available everywhereNot for high temperature, heavy shock, sliding contact, lubricant starvation or corrosionAll bearing series
100Cr6 martensitic, class S0Up to 62 HRC; over +150 °CSame as SN, with size stability at higher temperatureSame limits as SN for shock, sliding, starvation and corrosionAll bearing series
100Cr6 martensitic, class S1Up to 62 HRC; over +200 °CSame as SN, stable at the highest standard temperature classLower resistance to shock and to particle overrolling than the referenceSmall combustion engines; fan bearing supports in steel mills
100Cr6 bainitic, class S1Up to 62 HRC; over +200 °CHard, wear resistant, very good overrolling resistance; compressive stresses in the surface zone make cracks much less likely even with surface damageNot for corrosion or lubricant starvationRoller bearings with high sliding contact; bucket wheel excavators; tram wheelsets
St4 low-carbon steel, case hardenedUp to 62 HRC; to about +120 °CUniversal for small parts; good formability; good price and performance in large volumes of formed partsComparatively soft core, so lower fatigue strengthDrawn-cup needle roller bearings; universal joints; motorcycle swing arms

Case-hardened and carbonitrided steels

A hard surface over a tough core, or a surface with retained austenite. These are the steels for dirty oil, poor lubrication, shock loads and large bearings.

MaterialHardness and temperatureStrengthsLimitsTypical uses
100CrMnSi6-4, modified martensiticUp to 65 HRC; about 15% retained austenite; to about +120 °C (higher for short periods)High hardness and wear resistance; same fatigue strength in particle overrolling as carbonitrided 100Cr6 at a better priceHigh shock loads; sliding contact; corrosionSteel production; passenger car gearboxes
100CrMnSi6-4, carbonitrided66 HRC outer layer (62 + 4); more retained austeniteMuch higher resistance to surface damage; longer life in poor lubrication and where contamination risk is highHigh shock loads; corrosionHydraulic axial piston motor output shafts; construction and agricultural gearboxes
Case-hardening steel (17MnCr5, 17CrNiMo7-6), carburised and hardened64 HRC hard surface, tough core; to about +120 °CCompressive residual stresses in the surface; higher fracture resistance under shock or surface damage; less crack growth from damageCorrosion; temperature above +120 °CMedium and large bearings: wind turbine main rotor bearings, heavy truck wheel bearings
Case-hardening steel, carbonitridedUp to 65 HRC; to about +120 °C (higher for short periods)Very high wear resistance; higher dynamic load carrying capacity in poor lubrication; resists particle overrollingCorrosionSteel rolling mill bearings; wind power gearboxes

Corrosion-resistant steels

Where water, washdown, process media or weak acids would ruin a normal steel, and where a seal is costly or impossible.

MaterialHardness and temperatureStrengthsLimitsTypical uses
Nitrogen-alloyed corrosion-resistant steel (X30CrMoN15-1), martensiticUp to 62 HRC; to about +150 °CHigh load capacity, high fatigue life, very good corrosion resistance; allows costly seals to be left out; works with media lubrication and dry runningCorrosion by strong acidsMachine tool spindles; process pumps
Corrosion-resistant case-hardened nitrogen steelUp to 62 HRC hard surface, tough core; over +180 °CVery good resistance to overrolling and to corrosion; suited to lubricant starvation, first lubrication and dry runningStrong acidsBottle filling plant; inline skates
Austenitic stainless (X5CrNi18-10, AISI 304), carburisedThin hard layer of about 58 HRC with tough core; rings over 300 mm and loads over 2,000 MPaNon-magnetic; excellent resistance to media; no shielding neededLow hardness against martensitic steels, so lower fatigue strengthButterfly valve positioning; gimbal mountings

High-temperature and aerospace steels

Tool steels and nitrided steels that keep hardness far above the limit of 100Cr6, with very high speeds and little cooling.

MaterialHardness and temperatureStrengthsLimitsTypical uses
M50 tool steel, vacuum remelted, martensiticUp to 64 HRC; +350 to +400 °CThermally stable with increased toughness; needs little cooling; prevents premature failureCorrosion; extremely high centrifugal stressesAircraft engine main shaft bearings
M50NiL, case hardenedSurface up to 64 HRC; +350 to +400 °C; residual compressive stressesThermal stability with much higher toughness and fracture resistance; for very high speedsCorrosionAircraft engine main shaft bearings at extreme speed
M50NiL, duplex hardened (carburised, hardened and nitrided)Surface up to 70 HRC; +350 to +400 °CHigher fracture resistance, very good wear resistance, very good tolerance of damage after particle overrollingCorrosionAircraft engines at extreme speed
32CrMoV13, nitridedUp to 64 HRC; stable to +350 °C; nitriding depth over 0.6 mm; outside diameter up to about 160 mmHigh fatigue strength above +150 °C; good overrolling resistance even with starvation; resists surface damage by particles and false brinellingSize limited to about 160 mm outside diameterAircraft engine and other bearings under thermal load
Powder-metallurgy high-speed steelUp to 66 HRC; heat resistantHigh static and dynamic load capacity, wear and heat resistance; robust against brinelling, lubricant starvation and particle overrollingCorrosive attackMachine tool spindle bearings; engine components
Hard metal (cemented carbide with metallic binder)Above 1,300 HV; components up to 400 mm; wide temperature swingsVery high heat resistance, modulus of elasticity, wear and corrosion resistance; non-magnetic; allows ambient media in place of oil lubrication; dry runningSize limit about 400 mm; costOcean energy generation; pumps and compressors

Ceramic rolling elements and hybrid bearings

Steel rings with ceramic balls or rollers. Ceramic is hard, light, non-magnetic and an electrical insulator, and it runs with very little friction.

MaterialHardness and temperatureStrengthsLimitsTypical uses
Silicon nitride Si3N4, hot isostatically pressedAbout 1,500 HV; very low density; usable to about +700 °C; used with steel ringsHybrid bearings with much higher load capacity than ZrO2; with matched rings (nitrogen steel or carbonitrided) a much higher rating life even under high load; lower mass; very high speed; current insulation; less friction and longer grease lifeNormally used only as rolling elements against steel rings; higher costMachine tool spindles; food industry
Zirconium oxide ZrO2About 1,400 HV; density between Si3N4 and steel; usable to about +600 °C; thermal expansion close to steelCurrent insulation, wear resistance, lower friction; first lubrication; usually cheaper than Si3N4Contact pressures over 1,500 MPa; suited to low loadsElectric window motors in cars; food technology

Which material for which problem

Your problemWhat to look at
Ordinary duty, normal temperature100Cr6 martensitic, class SN or S0: the reference, with the best price and availability
Operating temperature above +150 °CHeat-stabilised rings (class S0 to S3 in the bearing number), then tool steels, nitrided 32CrMoV13 or ceramics above about +250 °C
Dirty oil or grease, particles in the lubricantCarbonitrided steel or steel with retained austenite; a hybrid bearing is another route
Shock loads or surface damage riskCase-hardened steel or bainitic steel: compressive stresses slow crack growth
Sliding or slippage (skidding rollers)Bainitic, carbonitrided, duplex or nitrided steels, or ceramic rolling elements
Water, washdown or process mediaNitrogen-alloyed corrosion-resistant steels, or ceramic or hard-metal parts for the harshest media
Starvation or dry runningCorrosion-resistant nitrogen steel, hard metal, or a hybrid bearing
Current through the bearing (inverter drives)Ceramic rolling elements (a hybrid bearing) or an insulated bearing; see the electrical damage pages
Very high speedHybrid bearings with ceramic balls, or tool steels, because the lower mass cuts centrifugal load
Non-magnetic dutyAustenitic stainless, hard metal or ceramic
Takeaway. A better material is a repair for a cause you cannot remove. Where dirt, water or heat can be cut at the source, do that first, then choose the steel for what is left.

Questions

What do the SN, S0 and S1 classes mean?

They are heat-stabilisation classes for the rings. SN is the standard class for service to about +120 °C, S0 holds size up to about +150 °C and S1 up to about +200 °C. Higher classes (S2, S3) go to about +250 °C and +300 °C. A bearing run hotter than its class can grow and lose clearance.

When is a hybrid ceramic bearing worth the extra cost?

When you need very high speed, protection from electric current through the bearing, longer grease life or tolerance of poor lubrication. Ceramic balls or rollers are hard and light, run cooler and do not carry current. They cost more than an all-steel bearing.

Which steel is best when the lubricant is dirty?

Carbonitrided steels, and steels with controlled retained austenite, tolerate hard particles in the oil or grease better than the standard steel. Cleaning the lubricant and sealing better still comes first.

Can a corrosion-resistant steel replace seals?

In some wet or media-lubricated duties a nitrogen-alloyed corrosion-resistant steel allows seals to be left out, but it has limits in strong acids. Check the medium before you decide.

Put it to work in the tool